Specifications
Product Data
ASTM C1364: Architectural Cast Stone
Mix Design
| Cement |
ASTM C150 Portland Type 1 |
94lbs. |
| Fine Aggregate: |
ASTM C33 Mortar Sand |
3.29 cubic feet |
| Water |
Potable (City of Fredericksburg) |
3 gallons |
| Admixture |
Plasticizer/Densifier |
12 ounces |
| Design Strength |
7500 P.S.I. |
| Yeild |
2.25 c.f. (compacted product) |
ASTM C1194: Compressive Strength of Architectural Cast Stone
Results of testing by Mactec Consulting and Engineering of Georgia, Inc., February 2003
| Specimen Identification |
Length (in.) |
Width (in.) |
Area (sq.in.) |
Load (lbs.) |
Compressive Strength |
| 1 |
2.079 |
1.97 |
4.1 |
32740 |
7985 |
| 2 |
1.984 |
2.075 |
4.117 |
36580 |
8886 |
| 3 |
1.961 |
1.994 |
3.91 |
33040 |
8450 |
|
|
|
|
Average |
8440 |
ASTM C1195: Absorption of Architectural Cast Stone, Method A
Results of testing by Mactec Consulting and Engineering of Georgia, Inc., February 2003
| Specimen Identification |
Test Weight (g) |
Test Results Absorption % |
| Oven Dry |
Saturated Surface Dry |
| 1 |
276.25 |
289.62 |
4.80% |
| 2 |
272.46 |
285.65 |
4.80% |
| 3 |
253.56 |
268.25 |
5.80% |
| TEMP. OF H2O, C: 23.0 |
AVERAGE |
5.20% |
ASTM C666: Resistance of Concrete to Rapid Freezing & Thawing
Results of Testing by Froehling & Robertson, Inc. April 2001
| Number of Cycles |
Weight (AVG. of 3 bars) |
Relative Modulus (AVG.) |
| 0 |
19.3 |
100 |
| 40 |
19.9 |
100 |
| 100 |
20 |
94.7 |
| 163 |
20 |
88.6 |
| 202 |
20 |
88.4 |
| 259 |
19.8 |
83.5 |
| 300 |
19.7 |
83.1 |
|
DF=83 CWL (LESS THAN 5%) NO EVIDENCE OF SIGNIFICANT SPALLING @ 300 CYCLES
|